Haynes® 188 alloy is a cobalt-nickel-chromium-tungsten alloy that possesses excellent strength and corrosion resistance at elevated temperatures.
| Composition | UNS N07001 % |
| Carbone | 0.1 |
| Manganèse | 1.25 max |
| Silicium | 0.35 |
| Chrome | 22 |
| Tungstène | 14 |
| Fer | 3 max |
| Cobalt | 39 balance |
| Lanthanum | 0.03 |
| Bore | 0.02 max |
| Nickel | 22.00 |
| Métrique | Anglais | |
| Densité | 8.98 g/cm³ | 0.324 lbs/in³ |
| Modulus of elasticity | 232 GPa | 33.7 mpsi |
| Electrical resistivity | 101.0 µohms/m | 39.6 µohms/in |
| Thermal conductivity | 10.4 W/m-K | 72 Btu-in/ft²hr-°F |
*values calculated at room temperature
| Cold worked % | Yield strength | Ultimate tensile strength | Elongation % |
| 0 | 938 MPa [136 ksi] | 1324 MPa [192 ksi] | 34 |
| 20 | 1110 MPa [161 ksi] | 1544 MPa [224 ksi] | 5.6 |
| 37 | 1641 MPa [238 ksi] | 2013 MPa [292 ksi] | 4.1 |
| 50 | 1813 MPa [263 ksi] | 2165 MPa [314 ksi] | 3.3 |
All data represent results from a 25.4 cm [10 in] test gauge length. Values are typical and may not represent all diameters. Test method will affect results.